- Home
- Guides
- PP with 30% glass fibre: reading the PP-GF30 datasheet
PP with 30% glass fibre: reading the PP-GF30 datasheet
Polypropylene with 30% glass fibre is for a part that must stay stiff and keep its shape under load and heat. Epic supplies two grades: PP-GF30 N and PP-GF30 GN. This guide explains what each datasheet row says and how to use it when choosing.
Values of the two grades
| Property | Test method | PP-GF30 N | PP-GF30 GN |
|---|---|---|---|
| Density (g/cm³) | ISO 1183 | 1.12 | 1.09 |
| Tensile stress at break (MPa) | ISO 527 | min. 70 | min. 70 |
| Tensile strain at break (%) | ISO 527 | 4.5 | 4.5 |
| Charpy notched impact, 23 °C (kJ/m²) | ISO 179 | min. 7 | min. 9 |
| Charpy unnotched impact, 23 °C (kJ/m²) | ISO 179 | 65 | 70 |
| Heat deflection temperature, 1.8 MPa (°C) | ISO 75 | 140 | 140 |
| Melting point (°C) | ISO 3146 | 165 | 165 |
| Moisture (%) | ISO 960 | below 0.2 | below 0.2 |
The values are typical, not a guaranteed specification; the material is a 4 to 5 mm granule.
What does each row mean?
- Density 1.12 or 1.09: with the same mould the part comes out heavier than in plain polypropylene, so compare prices as cost per part, not per kilogram: the real cost of granule.
- Tensile stress at least 70 MPa and strain 4.5%: the material is strong and stiff but stretches little before it breaks; the part design must allow for this.
- Charpy impact: shows how much energy the material absorbs in an impact. The notched test is the most severe case (a sharp corner or a weld line in the part); on this row GN is at least 9 and N at least 7.
- Heat deflection temperature 140 °C at 1.8 MPa: the temperature at which the material starts to bend under a set load; it is the main measure for a part that carries load when hot.
- Moisture below 0.2%: the moisture limit of the ready granule; if the bag has been left open, dry it before production (granule moisture and drying).
Injection moulding conditions
| Parameter | Value |
|---|---|
| Drying | 80 °C, 2 to 4 hours |
| Feed zone temperature | 60 to 70 °C |
| Melt temperature | 200 to 240 °C |
| Mould temperature | 20 to 50 °C (30 to 50 for reinforced grades) |
| Injection pressure | 55 to 65 MPa |
| Holding pressure | 50 to 60 MPa |
| Back pressure · injection speed | low · medium |
Packing: 25 kg bags; store in a dry, dust-free place at room temperature.
Choosing
If impact (especially at corners and notches) and a lower density matter more, check the GN rows against your needs; if a density of 1.12 is acceptable for the part, N has the same tensile and heat resistance. For final confirmation, run a small trial on your own mould: the values above are laboratory conditions, and part behaviour also depends on design and process.
Datasheets with the Epic letterhead and the full table are on the Persian page polypropylene with 30% glass fibre · an introduction to reinforced polypropylene: talc, carbonate and glass fibre · reading a datasheet: guide.
Questions
What is the difference between PP-GF30 N and GN?
On the datasheets, GN has a lower density (1.09 against 1.12) and higher Charpy impact; tensile stress and heat deflection are the same.
Are these guaranteed values?
No. They are typical values; confirm the batch datasheet and run a small trial on your mould.
Do I need to dry it before moulding?
If the bag has been left open, yes: 80 °C for 2 to 4 hours.
For a datasheet or sample contact Epic Polymer: +98 919 212 4919 · WhatsApp.